Izici:

I-AWS A5.1 E6013(J421) iyi-electrode yohlobo lwe-rutile. Ingashiselwa kokubili umthombo wamandla we-AC kanye ne-DC futhi ingaba ngeyazo zonke izikhundla. Isebenza kahle kakhulu ngokushiselwa njenge-arc ezinzile, i-spatter encane, isusa kalula i-slag kanye nekhono lokubuyisela emuva njll. I-electrode ye-Rutile-cellulosic enekhono elihle lokushiselwa kuzo zonke izikhundla kufaka phakathi phansi okuqondile. Ikhono elihle kakhulu lokuhlanganisa igebe kanye nokushaya i-arc. Yokushisela i-tack kanye nokulingana komthwalo. Inhloso ejwayelekile yezimboni kanye nokuhweba, ukuhlanganisa kanye nokushisela esitolo.

Ukwakheka Kwamakhemikhali Kwazo Zonke Izinsimbi Ezihlanganisiwe: (%)
Ukwakheka Kwamakhemikhali C Mn Si S P Ni Cr Mo V
Izidingo ≤0.10 0.32-0.55 ≤0.30 ≤0.030 ≤0.035 ≤0.30 ≤0.20 ≤0.30 ≤0.08
Imiphumela Ejwayelekile 0.08 0.37 0.18 0.020 0.025 0.030 0.035 0.005 0.004
Izakhiwo Zemishini Zensimbi Egciniwe
Into Yokuhlola I-Rm (N/mm2) I-Rel (N/mm2) A (%) I-KV2(J) 0℃
Izidingo 440-560 ≥355 ≥22 ≥47
Imiphumela Ejwayelekile 500 430 27 80
I-AWS A5.1 E6013 ifanele izakhiwo zokushisela ezenziwe ngensimbi ephansi yekhabhoni, isebenza kahle kakhulu ekushiseleni amapuleti ensimbi amancane namakhulu amancane futhi isebenza kahle kakhulu esimweni esidinga ukubukeka okuhle nokuhlanzekile kobuhlalu.

Isikhundla Sokushisela:

I-PA, i-PB, i-PC, i-PD, i-PE, i-PF

Inkomba Yamanje (DC)
Ububanzi φ2.0 φ2.5 φ3.2 φ4.0 φ5.0
I-Amperage 40 ~ 70 50 ~ 90 80~ 130 150 ~ 210 180 ~ 240

Ukunakwa:

Ngokuvamile, don'Akudingeki ukuthi womise kabusha i-electrode ngaphambi kokuyishisela. Uma ithintekile ngenxa yomswakama, kufanele yomise kabusha ku-150℃-170℃ihora elingu-0.5-1.