I-AWS ENiCu-7 Nickel Alloy Welding Rods Ni70Cu30 Nickel Based Welding Electrodes Manual Metal Arc Electrodes

Incazelo emfushane:

I-Ni202 (AWS ENiCu-7) iyi-electrode ye-Ni70Cu30 Monel alloy ene-titanium calcium coating.Ingasetshenziselwa kokubili i-AC ne-DC.


Imininingwane Yomkhiqizo

Omaka bomkhiqizo

I-Nickel ne-Nickel Alloy Welding Electrode

Ni202                                                     

I-GB/T EN4060

I-AWS A5.11 ENiCu-7

Incazelo: I-Ni202 iyi-electrode ye-Ni70Cu30 Monel alloy ene-titanium calcium coating.Ingasetshenziswa kokubili i-AC ne-DC.Insimbi efakiwe inokumelana nokuqhekeka okuhle ngenxa yokuqukethwe okufanele kwe-manganese ne-niobium.Inokusebenza okuhle kakhulu kokushisela okunokushiswa kwe-arc okuzinzile, i-spatter encane, ukususa i-slag kalula, kanye ne-weld enhle.

Isicelo: Isetshenziselwa ukushisela i-nickel-copper alloy kanye nensimbi engafani, futhi ingasetshenziswa njengento yokumbondela yesikhashana.

 

Ukwakheka kwamakhemikhali ensimbi ye-weld(%):

C

Mn

Fe

Si

Nb

Al

Ti

Cu

Ni

S

P

≤0.15

≤4.0

≤2.5

≤1.5

≤2.5

≤1.0

≤1.0

27.0 ~ 34.0

≥62.0

≤0.015

≤0.020

 

Izici zemishini ye-weld metal:

Into yokuhlola

Amandla aqinile

Mpa

Amandla esivuno

Mpa

Ukwelula

%

Kuqinisekisiwe

≥480

≥200

≥27

 

Okwamanje okunconyiwe:

Ububanzi benduku

(mm)

2.5

3.2

4.0

Welding current

(A)

50 ~ 80

90 ~ 110

110 ~ 150

 

Isaziso:

1. I-electrode kufanele ibhakwe ihora elingu-1 endaweni engaba ngu-250 ℃ ngaphambi kokusebenza kokushisela;